EN10113 S420ML steel plate/sheet,EN10113 S420ML steel plate/sheet, under EN standard, we can regard S420ML steel plate/sheet for Fine-grain structural steels, thermomechanically rolled steel.
EN10113 S420ML is a technical delivery conditions for thermomechanical rolled weldable fine grain structural steels.S means the structural steel, M means the delivery condition.Capital letter L for the quality with specified minimum values of values of impact energy at temperature not lower than -50 degree.It is equal to SEW083 TStE420TM,NFA36-201 E420FP and ASTM A633Gr.E
S420ML EN 10113-3 Number:1.8836 |
Comparision of steel grades | |
SEW 083 | TStE 420 TM | |
NFA 36-201 | E 420 FP | |
UNI 7382 | - | |
BS 4360 | - | |
ASTM | A 633 Gr.E |
Chemical Composition of EN S420ML steel
Grade | C max |
Si max |
Mn max |
P max |
S max |
N max |
AL max |
Nb max |
V max |
Ti max |
Cr max |
Ni max |
Mo max |
Cu max |
CEV max |
S420ML | 0.16 % |
0.50 % |
1.70 % |
0.025 % |
0.02 % |
0.02 % |
0.02 % |
0.05 % |
0.12 % |
0.05 % |
0.30 % |
0.80 % |
0.20 % |
0.55 % |
0.47 % |
Mechnical Properties of EN S420ML steel
Temperature | -50 | -40 | -30 | -20 | -10 | 0 | 20 |
Notch impact test. Min. absorbed energy | 27 | 31 | 40 | 47 | 51 | 55 | 63 |
Nominal thickness(mm) | to 16 | 16-40 | 40-63 | 63-80 | 80-100 | 100-120 |
ReH-Minimun yield strength(Mpa) | 420 | 400 | 390 | 380 | 370 | 365 |
Nominal thickness(mm) | to 40 | 40-63 | 63-80 | 80-100 | 100-120 |
Rm-Tensile strength(Mpa) | 520-680 | 500-660 | 480-640 | 470-630 | 460-620 |
Nominal thickness(mm) | - | ||||
A-Minimum elongation Lo=5,65√So(%) |
19 |
Source: