S235JR steel plate, under EN10025 standard S235JR steel plate, under EN10025 standard, we can regard S235JR steel plate as Carbon and low alloy steel
S235JR steel plate is one mainly of Carbon and low alloy steel, S235JR steel plate is a type of steel sheet under EN standard which is used to build ship, bridge, belongs to high strength sheet. S235JR is equivalent to DIN:ST37-2,JIS:SS400,ASTM:A283C and UNI:FE360B
S235JR DIN EN 10025-2Number: 1.0037 | Comparison of steel grades | |
EN10025:1990 | FE 360 B | |
DIN17100 | ST37-2 | |
NFA 35-501 | E24-2 | |
JIS3101 | SS400 | |
ASTM | A283C | |
UNI7070 | FE 360 B |
S235JR Chemical analysis -% by mass*
Chemical elements | C≤ 16mm max | C>16mm max | Si max |
Mn max | P max. |
S max. |
%,by mass | 0.17 | 0.20 | -- | 1.40 | 0.045 | 0.045 |
thickness | Yield Strength ReH[N/mm2] transv.min. | Tensile Strength Rm [N/mm2]transv. | Fracture Elongation[%] transv. min. | Notch Impact Energy1)Ch Vcomplete samplelongitud. min [J] |
t≤ 16mm t >16mm | 235 225 | 20 degree 27J | ||
t < 3mm t ≥ 3mm | 360-510 340-470 | |||
Up to 1.5mm 1.51-2.00mm 2.01-2.50mm 2.51-2.99mm ≥3mm | 16 17 18 19 24 |
SS400 steel plate, JIS3101 SS400 steel plate, under JIS3101 standard, we can regard SS400 steel plate as Carbon and low alloy steel SS400 steel plate is one mainly of Carbon and low alloy steel, SS400 steel plate would be used to built containers which can bear low temperature sea water.When customers order SS400 steel plate from us,our mill should be roll them completely according to JIS3101 specifications,the mill would issue original Mill test certificates before taking delivery for checking
SS400 steel plate Chemical analysis -% by mass*
Chemical elements | C≤ 16mm max | C>16mm max | Si max |
Mn max | P max. |
S max. |
%,by mass | 0.17 | 0.20 | -- | 1.40 | 0.045 | 0.045 |
SS400 steel sheet Mechanical properties
thickness | Yield StrengthReH[N/mm2] transv.min. | TensileStrengthRm[N/mm2]transv. | Fracture Elongation[%]transv. min. | Notch Impact Energy1)Ch Vcomplete samplelongitud. min [J] |
t≤ 16mm t >16mm | 235 225 | 20 degree 27J | ||
t < 3mm t ≥ 3mm | 360-510 340-470 | |||
Up to 1.5mm 1.51-2.00mm 2.01-2.50mm 2.51-2.99mm ≥ 3mm | 16 17 18 19 24 |
ASTM A36 | ||||
Structural Quality ASTM A36 General Description - One of the most widely used carbon steel plate specifications for constuctional purposes. (The specification also covers carbon steel shapes and bars.) |
||||
ASTM A36 Mechanical Properties | ||||
Yield Point, Min., Tensile Strength, Plates over 8" - Yield Point |
ksi 36 ksi 58/80 32 ksi |
|||
ASTM A36 Chemical Requirements - Percent, % (Heat Analysis) | ||||
Thickness, In Inches to 3/4" |
Over 3/4" To 1-1/2" | Over 1-1/2" To 2-1/2" | Over 2-1/2" To 4" | Over 4" |
Carbon, max. 0.25 | 0.25 | 0.26 | 0.27 | 0.29 |
Manganese - | 0.80/1.20 | 0.80/1.20 | 0.85/1.20 | 0.85/1.20 |
Silicon - | - | 0.15/0.40 | 0.15/0.40 | 0.15/0.40 |
Copper 0.20 minimum maybe be specified to improve atmospheric corrosion resistance. ASTM A36 Applications - Used in riveted, bolted, or welded construction of buildings, bridges and for general stuctural purposes. |