Grade
|
C(%)
Min-Max
|
Si(%)
Min-Max
|
Mn(%)
Min-Max
|
P(%)
Max
|
S(%)
Max
|
Cr(%)
Min-Max
|
C22
|
0.17-0.24
|
0.15-0.35
|
0.40-0.70
|
0.025
|
0.025
|
0.20-0.40
|
C35
|
0.32-0.39
|
0.15-0.35
|
0.50-0.80
|
0.025
|
0.025
|
0.20-0.40
|
C45
|
0.42-0.50
|
0.15-0.35
|
0.50-0.80
|
0.025
|
0.025
|
0.20-0.40
|
C55
|
0.52-0.60
|
0.15-0.35
|
0.60-0.90
|
0.025
|
0.025
|
0.20-0.40
|
C60
|
0.57-0.65
|
0.15-0.35
|
0.60-0.90
|
0.025
|
0.025
|
0.20-0.40
|
C67
|
0.65-0.73
|
0.15-0.35
|
0.60-0.90
|
0.025
|
0.025
|
0.20-0.40
|
C75
|
0.70-0.80
|
0.15-0.35
|
0.60-0.90
|
0.025
|
0.025
|
0.20-0.40
|
Mechanical Properties
Grade
|
Condition
|
Yield
strength(MPa)
|
Tensile strength
(MPa)
|
Elonga-
tion
(%)
|
Hardness
HRC
|
Quenching
Temperature
(°C)
|
C22
|
|
360
|
510
|
28
|
|
-
|
|
280
|
420
|
30
|
|
||
C35
|
|
440
|
700
|
18
|
-
|
|
|
310
|
480
|
30
|
-
|
|
|
Rolled
|
|
1845
|
|
53
|
840
|
|
Annealed
|
|
1690
|
|
50
|
880
|
|
C45
|
Waterquenched
|
460
|
750
|
18
|
|
|
Oil quenched
|
330
|
540
|
30
|
|
|
|
|
|
2270
|
|
58
|
840
|
|
|
|
1980
|
|
55
|
880
|
|
C55
|
|
500
|
825
|
18
|
|
|
|
350
|
550
|
30
|
|
|
|
|
|
2510
|
|
61
|
805
|
|
|
|
2120
|
|
57
|
845
|
|
C60
|
|
540
|
875
|
17
|
|
|
|
370
|
580
|
29
|
|
|
|
|
|
2670
|
|
63
|
800
|
|
|
|
2430
|
|
60
|
840
|
|
C67
|
|
570
|
925
|
16
|
|
|
|
370
|
580
|
29
|
|
|
|
|
|
2920
|
|
66
|
790
|
|
|
|
2670
|
|
63
|
830
|
|
C75
|
|
600
|
1000
|
15
|
|
|
|
370
|
570
|
28
|
|
|
|
|
|
3000
|
|
67
|
785
|
|
|
|
2760
|
|
64
|
825
|
Welding
Source:
Tags: C45, C50, C55, C45, C50, C55, steel plate, C45, C50, C55, steel is high carbon steel for mould and wear resistance.